Bii o ṣe le ṣe ilọsiwaju awọn iwọn ilana simẹnti ti oṣuwọn spheroidization
Ipele spheroidization ti ile simẹnti simẹnti simẹnti simẹnti simẹnti ni a nilo lati de ipele 4 tabi loke, (iyẹn ni, oṣuwọn spheroidization jẹ 70%), oṣuwọn spheroidization ti o waye nipasẹ ipilẹ gbogbogbo jẹ nipa 85%. Ni awọn ọdun aipẹ, pẹlu idagbasoke iṣelọpọ nodular simẹnti irin, ni pataki ni awọn ile -iṣẹ pẹlu awọn ibeere giga fun iṣelọpọ simẹnti agbara afẹfẹ ati didara simẹnti, a nilo ipele spheroidization lati de ipele 2, iyẹn ni, oṣuwọn spheroidization de diẹ sii ju 90%. Ile-iṣẹ onkọwe ṣe itupalẹ ati ilọsiwaju spheroidization ati ilana inoculation ti a lo ni QT400-15, gẹgẹ bi oluranlowo spheroidizing ati inoculant, nitorinaa oṣuwọn spheroidization ti iron iron nodular de diẹ sii ju 90%.
1. Ilana iṣelọpọ atilẹba
Ilana iṣelọpọ atilẹba:
- Ohun elo mimu n gba ileru igbohunsafẹfẹ agbedemeji 2.0T ati ileru igbohunsafẹfẹ ile -iṣẹ 1.5T;
- Tiwqn ti QT400-15 omi irin aise jẹ ω (C) = 3.75%~ 3.95%, ω (Si) = 1.4%~ 1.7%, ω (Mn) ≤0.40%, ω (P) -0.07%, ω ( S)) ≤0.035%;
- Aṣoju spheroidizing ti a lo ninu itọju spheroidizing jẹ 1.3% si 1.5% RE3Mg8SiFe alloy;
- Inoculant ti a lo ninu itọju inoculation jẹ 0.7% ~ 0.9% 75SiFe-C alloy. Itọju spheroidizing gba awọn titẹ ni kia kia ati awọn ọna fifọ meji:
Ni akọkọ, 55% ~ 60% ti irin ni iṣelọpọ, lẹhinna spheroidizing ni a gbe jade, lẹhinna inoculant ti ṣafikun, lẹhinna iyoku omi omi irin naa ṣafikun.
Nitori ọna ibile ti spheroidization ati inoculation, oṣuwọn spheroidization ti a rii nipasẹ bulọọki idanwo simẹnti simẹnti kan pẹlu sisanra ti 25 mm ni gbogbogbo ni ayika 80%, iyẹn ni, ipele spheroidization jẹ 3rd.
2. Eto idanwo lati ni ilọsiwaju oṣuwọn spheroidization
Lati le pọ si oṣuwọn spheroidization, ipilẹṣẹ spheroidization atilẹba ati ilana inoculation ti ni ilọsiwaju. Awọn ọna akọkọ jẹ: jijẹ iye ti oluranlowo spheroidizing ati inoculant, ṣiṣe wẹ irin didan, ati itọju desulfurizing. Oṣuwọn spheroidization tun jẹ idanwo pẹlu ohun elo idanwo simẹnti simẹnti kan ti 25 mm. Ilana kan pato jẹ bi atẹle:
- (1) Ṣe itupalẹ idi fun oṣuwọn spheroidization kekere ti ilana atilẹba. A ro pe iye oluranlowo spheroidizing jẹ kekere, nitorinaa iye ti oluranlowo spheroidizing ti pọ si pọ si lati 1.3% si 1.4% si 1.7%, ṣugbọn oṣuwọn spheroidizing ko pade awọn ibeere. . (2) Amọran miiran ni pe oṣuwọn spheroidization kekere le fa nipasẹ oyun ti ko dara tabi idinku irọyin. Nitorinaa, idanwo naa pọ si iwọn lilo lati 0.7% si 0.9% si 1.1%, ati oṣuwọn spheroidization ko pade awọn ibeere.
- (3) Tẹsiwaju lati ṣe itupalẹ ati gbagbọ pe awọn ifisi diẹ sii wa ninu irin didà ati awọn eroja kikọlu spheroidization giga le jẹ idi ti oṣuwọn spheroidization kekere. Nitorinaa, iwẹnumọ iwọn otutu giga ti irin didà ni a ṣe. Iwọn iwọn isọdọmọ iwọn otutu ti o ga ni gbogbo iṣakoso ni 1500 ± 10 ° C, ṣugbọn oṣuwọn spheroidization rẹ ko ti kọja 90%.
- (4) Iwọn giga ti ω (S) ni pataki njẹ iwọn lilo spheroidizing ati yiyara idinku ti spheroidization. Nitorinaa, itọju desulfurization ti pọ si lati dinku iye omi irin akọkọ ω (S) lati 0.035%si kere si 0.020%, ṣugbọn oṣuwọn spheroidization tun jẹ Nikan de 86%. Awọn abajade idanwo ti awọn ero mẹrin ti o wa loke ni a fihan ni Tabili 1. Eto ati awọn ohun-ini ẹrọ ti dina idanwo ti o ni irufẹ ko pade awọn ibeere.
3. Eto ilọsiwaju ti o kẹhin gba
3.1 Awọn igbese ilọsiwaju ni pato
- Awọn ohun elo aise jẹ irin ẹlẹdẹ, rustless tabi kere si rusty aloku ati awọn ohun elo imunna;
- Desulfurization ti aise didà irin nipa fifi soda eeru (Na2CO3) si ileru;
- Lo aṣoju Foseco 390 lati ṣaju deoxidize ninu apo;
- Itọju Spheroidizing pẹlu Fozco Nodulizer;
- Lilo carbide silikoni ati ferrosilicon idapo inoculation.
Iṣakoso akopọ irin ti didà atilẹba ti ilana tuntun: ω (C) = (3.70% ~ 3.90%, ω (Si) = 0.80% ~ 1.20% [simẹnti ω (Si ipari) = 2.60% ~ 3.00%], ω ( Mn) ≤ 0.30%, ω (P) ≤0.05%, ω (S) ≤0.02%. Nigbati irin didan atilẹba ω (S) ti kọja 0.02%, eeru omi onisuga ile -iṣẹ ni a lo fun desulfurization ni iwaju ileru, nitori ifura desulfurization jẹ ifura endothermic, Iwọn otutu desulfurization ni a nilo lati ṣakoso ni ayika 1500 ° C, ati iye eeru soda ti a ṣafikun ni iṣakoso ni 1.5% ~ 2.5% ni ibamu si iye ω (S) lakoko yo ninu ileru .
Ni akoko kanna, package itọju spheroidizing gba package itọju iru idido omi arinrin kan. Ni akọkọ, ṣafikun 1.7% ti Foseco NODALLOY7RE aṣoju spheroidizing aṣoju si ẹgbẹ ti idido ni isalẹ ti package, fẹlẹfẹlẹ ati iwapọ, ati lo 0.2% carbide silikoni lulú ati 0.3% kekere Awọn olopobobo 75SiFe ti bo pẹlu fẹlẹfẹlẹ kan lẹkan , ati lẹhin tamping, o ti bo pẹlu irin titẹ, ati 0.3% Foseke 390 inoculant ti wa ni afikun si apa keji ti irin ladle didà. Nigbati o ba tẹ irin, 55% ~ 60% ti iwọn irin didà lapapọ ni a kọkọ ṣan. Lẹhin ti iṣesi spheroidizing ti pari, 1.2% 75SiFe-C inoculant ti wa ni afikun ati irin didan ti o ku ti ṣan, ati pe a ti da slag naa.
3.2 Awọn abajade idanwo
Tiwqn ti irin didan atilẹba ṣaaju ati lẹhin desulfurization, awọn ohun-ini ẹrọ ati igbekalẹ irin-irin ti 25mm idena simẹnti simẹnti simẹnti ẹyọkan, ati ọna igbelewọn ti oṣuwọn spheroidization ni ọna irin-irin ni a rii laifọwọyi nipasẹ eto onínọmbà aworan metallographic. .
4. Onínọmbà abajade
4.1 Ipa ti awọn eroja akọkọ lori oṣuwọn spheroidization
- C, Si: C le ṣe agbega iṣapẹẹrẹ ati dinku ihuwasi ti ẹnu funfun, ṣugbọn iye giga ti ω (C) yoo jẹ ki CE ga pupọ ati irọrun fa graphite lati leefofo, ni iṣakoso ni gbogbogbo ni 3.7%~ 3.9%. Si le teramo agbara ayaworan ati imukuro simenti. Nigbati a ba ṣafikun Si bi alailagbara, o le dinku agbara supercooling ti irin didà Lati le mu ilọsiwaju inoculation pọ si, iye ω (Si) ninu irin didan atilẹba ti dinku lati 1.3% si 1.5% si 0.8% si 1.2%, ati iye ti ω (Si ikẹhin) ni iṣakoso ni 2.60%si 3.00%.
- Mn: Lakoko ilana kristali, Mn ṣe alekun ifarahan ti irin simẹnti si apọju ati ṣe agbekalẹ dida awọn carbides (FeMn) 3C. Ninu ilana iyipada eutectoid, Mn dinku iwọn otutu iyipada eutectoid, ṣe iduroṣinṣin ati tunṣe pearlite. Mn ko ni ipa pupọ lori oṣuwọn spheroidization. Nitori ipa ti awọn ohun elo aise, iṣakoso gbogbogbo ω (Mn) <0.30%.
- P: Nigbati ω (P) <0.05%, o jẹ tiotuka ni Fe, ati pe o nira lati ṣe eutectic irawọ owurọ, eyiti ko ni ipa diẹ lori oṣuwọn spheroidization ti irin ductile.
- S: S jẹ nkan ti ko ni iyalẹnu. S n gba Mg ati RE ninu oluranlowo spheroidizing lakoko ifaagun spheroidizing, idiwọ idiwọ ati idinku oṣuwọn spheroidizing. Sulfide slag yoo tun pada si imi -ọjọ ṣaaju ki irin didà ti fẹsẹmulẹ, lẹẹkansi n gba awọn eroja spheroidizing, yiyara idinku ti spheroidization, ati ni ipa siwaju oṣuwọn spheroidizing. Lati le ṣaṣeyọri oṣuwọn spheroidization giga, iye ω (S) ninu irin aise yẹ ki o dinku si kere ju 0.02%.
4.2 Itọju desulfurization
Lẹhin ti idiyele ti yo, mu awọn ayẹwo ati itupalẹ akopọ kemikali. Nigbati iye ω (S) ba ga ju 0.02%, a nilo imukuro.
Ilana ti imukuro eeru soda ni: fi iye kan ti eeru soda sinu ladle, lo ṣiṣan irin didan lati ṣan ati aruwo, eeru soda ti bajẹ ni iwọn otutu giga, agbekalẹ ifesi jẹ Na2CO3 = Na2O+CO2 ↑: Na2O ti ipilẹṣẹ jẹ ninu irin didà lẹẹkansi Sulfuration ati dida Na2S, (Na2O) + [FeS] = (Na2S) + (FeO).
Na2CO3 ya sọtọ ati yanju CO2, ti o fa idamu iwa -ipa ti irin didà, eyiti o ṣe agbekalẹ ilana desulfurization. Soda ash slag jẹ irọrun lati ṣan ati leefofo loju omi ni iyara, ati akoko ifesi desulfurization kuru pupọ. Lẹhin desulfurization, o yẹ ki o yọ slag ni akoko, bibẹẹkọ yoo pada si imi -ọjọ. 4.3 Itọju iṣaaju deoxidation, itọju spheroidization ati itọju inoculation Foseke 390 oluranlowo idariji ṣe ipa ti itọju iṣaaju deoxidation ninu apo, ati ni akoko kanna pọ si mojuto ipilẹ eefin lẹẹdi ati nọmba awọn aaye lẹẹdi fun agbegbe kan, ati pe o tun le mu oṣuwọn gbigba ti Mg pọ si. Ni pataki ni ilọsiwaju agbara lati koju ipadasẹhin ati mu oṣuwọn spheroidization pọ si. Fochke inoculant ni ω (Si) = 60% ~ 70%, ω (Ca) = 0.4% ~ 2.0%, ω (Ba) = 7% ~ 11%, eyiti Ba le fa akoko isisẹ to munadoko sii. Ipele NODALLOY7RE ti Fozco Nodulizer ti yan, ati pe ω (Si) = 40%~ 50%, ω (Mg) = 7.0%~ 8.0%, ω (RE) = 0.3%~ 1.0%, ω (Ca) = 1.5 %~ 2.5%, ω (Al) <1.0%. Niwọn igba ti irin didan ti ngba desulfurization ati awọn itọju iṣaaju deoxidation, awọn eroja ti o jẹ awọn nodulizer ninu irin didà ti dinku pupọ, nitorinaa a ti yan nodulizer pẹlu iye kekere ti ω (RE) lati dinku ibajẹ ti spheroidal graphite morphology nipasẹ RE ; Apa akọkọ ti iṣe jẹ Mg; Ca ati Al le ṣe ipa kan ni okun isọdọmọ. Lilo carbide silikoni ati itọju idapo idapọmọra ferrosilicon, aaye yo ti silikoni carbide jẹ nipa 1600 ° C, ati pe eefin garafa ti pọ si nigba imuduro, ati awọn iwọn nla ti ferrosilicon ni a lo fun inoculation, eyiti o le ṣe idiwọ spheroidization lati idinku.
Ipari 5
Ni iṣelọpọ iron iron nodular ferritic, nigbati o nilo oṣuwọn spheroidization lati de ọdọ diẹ sii ju 90%, awọn iwọn atẹle le gba:
- (1) Yan idiyele didara to ga lati dinku awọn eroja de-spheroidization ninu idiyele naa.
- (2) Yan oluranlowo spheroidizing pẹlu iwọn kekere ti ω (RE) lati dinku ipa ti o bajẹ ti RE lori ẹkọ nipa ara ti lẹẹdi spheroidal.
- (3) Awọn akoonu ω (S) ti irin didan atilẹba yẹ ki o kere si 0.020%, eyiti o le dinku agbara ti awọn nodulizers, ni pataki awọn eroja ti ko ni agbara ti o jẹ nipasẹ imi -ọjọ keji ti slag sulfide.
- (4) Pre-deoxidize irin didà, mu nọmba awọn aaye lẹẹdi pọ si fun agbegbe kan, mu iwọn spheroidization pọ si, mu agbara pọ si pupọ lati koju ipadasẹhin, ati fa akoko isunmọ to munadoko.
- (5) Din iye ω (Si) ninu irin didan atilẹba, pọ si iye ti oluranlowo spheroidizing, inoculant ati awọn aṣoju idariji oriṣiriṣi, ati mu itọju inoculation lagbara.
Jọwọ tọju orisun ati adirẹsi ti nkan yii fun atunkọ: Bii o ṣe le ṣe ilọsiwaju awọn iwọn ilana simẹnti ti oṣuwọn spheroidization
Minghe Kú Simẹnti Company ti wa ni igbẹhin lati ṣe ati pese didara ati iṣẹ Awọn ẹya Simẹnti giga (irin awọn ẹya simẹnti ku ni ibiti o kun pẹlu Tinrin-Odi Kú Simẹnti,Gbona Iyẹwu Kú Simẹnti,Cold Iyẹwu Kú Simẹnti), Iṣẹ Yika (Iṣẹ Iṣẹ Simẹnti Kú,Machines Cnc,Mimu ṣiṣe, Itoju Itoju) .Iyi aṣa Aluminiomu simẹnti ku, magnẹsia tabi Zamak / zinc simẹnti ku ati awọn ibeere simẹnti miiran jẹ igbadun lati kan si wa.
Labẹ iṣakoso ti ISO9001 ati TS 16949, Gbogbo awọn ilana ni a ṣe nipasẹ awọn ọgọọgọrun ti awọn ẹrọ simẹnti ti o ku ti o ti ni ilọsiwaju, awọn ẹrọ axis 5, ati awọn ohun elo miiran, ti o wa lati awọn ẹrọ fifun si awọn ẹrọ fifọ Ultra Sonic. ẹgbẹ ti awọn ẹlẹrọ ti o ni iriri, awọn oniṣẹ ati awọn oluyẹwo lati jẹ ki apẹrẹ alabara ṣẹ.
Onigbọwọ olupese ti awọn adarọ ku. Awọn agbara pẹlu iyẹwu tutu aluminiomu awọn ẹya simẹnti lati 0.15 lbs. si 6 lbs., Iyipada iyara ti a ṣeto, ati sisẹ ẹrọ. Awọn iṣẹ ti a fi kun iye pẹlu didan, titaniji, deburring, fifa fifa shot, kikun, fifọ, fifọ, apejọ, ati irinṣẹ. Awọn ohun elo ti o ṣiṣẹ pẹlu pẹlu awọn irin bi 360, 380, 383, ati 413.
Zinc kú iranlowo apẹrẹ simẹnti / awọn iṣẹ ṣiṣe ẹrọ nigbakanna. Aṣa aṣa ti konge sinkii kú awọn adarọ ese. Awọn simẹnti kekere, awọn simẹnti ti o ku ti o ga julọ, awọn simẹnti mimu pupọ-ifaworanhan, awọn simẹnti mii aṣa, ẹyọ ku ati awọn simẹnti ku ti ominira ati awọn simẹnti ti a fi edidi le ti ṣelọpọ. A le ṣe awọn simẹnti ni awọn gigun ati awọn ibú to 24 ni. Ni +/- 0.0005 ni ifarada.
ISO 9001: Oluṣowo ti a fọwọsi 2015 ti iṣuu magnẹsia ti a fi silẹ, Awọn agbara pẹlu iṣuu magnẹsia titẹ giga ti o n ju simẹnti iyẹwu 200 pupọ & iyẹwu tutu 3000, apẹrẹ irinṣẹ, didan, mimu, ẹrọ, lulú & kikun omi, QA kikun pẹlu awọn agbara CMM , apejọ, apoti & ifijiṣẹ.
ITAF16949 ifọwọsi. Iṣẹ Afikun Simẹnti Pẹlu awọn simẹnti idoko,simẹnti iyanrin,Sisun walẹ, Sisọnu Foomu Foomu,Simẹnti Centrifugal,Simẹnti Igbale,Yẹ m Simẹnti, .Awọn agbara pẹlu EDI, iranlọwọ ti imọ-ẹrọ, awoṣe didi ati ṣiṣe atẹle.
Awọn ile-iṣẹ Simẹnti Awọn Ijinlẹ Ọran Awọn ẹya fun: Awọn ọkọ ayọkẹlẹ, Awọn keke, Ọkọ ofurufu, Awọn ohun elo orin, Watercraft, Awọn ẹrọ Optical, Awọn sensosi, Awọn awoṣe, Awọn ẹrọ itanna, Awọn apade, Awọn agogo, Ẹrọ, Awọn ẹrọ, Awọn ohun-ọṣọ, Awọn ohun-ọṣọ, Jigs, Telecom, Ina, Awọn ẹrọ Egbogi, Awọn ẹrọ aworan, Awọn roboti, Awọn ere ere, Ẹrọ ohun, Ohun elo ere idaraya, Irinṣẹ irinṣẹ, Awọn nkan isere ati diẹ sii.
Kini A le ṣe iranlọwọ fun ọ lati ṣe nigbamii?
Lọ Si oju-iwe akọọkan Fun Kú Simẹnti China
→Awọn ẹya ara Sisọ-Wa ohun ti a ti ṣe.
Tips Awọn imọran Ralated Nipa Kú Awọn iṣẹ Simẹnti
By Minghe Kú Simẹnti Ẹlẹda | Awọn ẹka: Awọn nkan iranlọwọ |awọn ohun elo ti Tags: Aluminiomu Simẹnti, Sinkii Simẹnti, Iṣuu magnẹsia, Pipe Titanium Pipes, Simẹnti Irin alagbara, irin, Idẹ Simẹnti,Idẹ Simẹnti,Fidio Simẹnti,Ile-iṣẹ Ile-iṣẹ,Casting Aluminiomu Die | Comments Pa